MCA (melamine cyanurate), is a non-halogen flame retardant with excellent performance.

The flame retardant mechanism of MCA is to encounter high temperature decarburization, the carbonized layer has the effect of heat insulation and oxygen barrier, and releases inert gas to play the role of flame retardant.

MCA flame retardants are widely used in flame retardant systems for engineering plastics, especially flame-retardant nylon, because of their low price, good flame-retardant effect, and no effect on the colour scheme of the material.

MCA flame retardants are thermally stable and can be used in processing temperatures of around 300 degrees, but MCA is prone to high temperature degradation and is particularly sensitive to pressure and shear.

Case 1.

A large injection molded product, with a large area and relatively thick, requires a high temperature and a long holding time during injection production.

The customer’s prototype was made of flame-retardant nylon PA66 and the flame-retardant used was MCA.

The injection molded parts always had splash-like patches near the glue inlet, which were radially distributed in the direction of melt flow. According to the master of the injection moulding plant, temperature adjustment was almost impossible to solve this problem. Later the material was changed to PA6, which is also MCA flame retardant, and the same problem still existed.

Case 2:

When producing MCA flame retardant nylon modified pelletizing, the temperature and machine speed parameters are stable. Due to the twin-screw machine blocking vacuum or the head mouth die blockage, causing MCA degradation, material foaming, yellowing, very easy to cause broken strips, material discoloration.

Case 3:

Production of MCA flame-retardant nylon on the twin-screw screw combination has a certain amount of attention. A production of glass-fiber reinforced nylon 65 twin-screw production line, the production of 15% content of flame retardant PA6, the phenomenon of foam yellowing, but also cannot be normal traction pulling strips. Even if the temperature is lowered to 230 degrees, the problem of yellowing foam still cannot be solved.

There are three sets of gear rings in the screw combination for glass fiber shearing and dispersion, so remove the three sets of gear rings and replace them with conveying elements to reduce the residence time of the melt in the barrel for fast, low-pressure extrusion. Alternatively, retain the original screw combination, open the head section, funnel one end of the screw and extrude according to the normal process.

Both processes can effectively solve the problem of yellowing foam in flame retardant nylon. The degradation of MCA flame retardant produces gas, and the relationship with mechanical shear or temperature is not obvious, but more sensitive to pressure and dwell time.

Based on the above knowledge, we can know that when producing MCA flame retardant nylon, we should pay attention to the following issues:

1. Try to avoid the production of large products, it is recommended to use it for small products and quick opening of the mould.

2. Modified pelletizing, attention should be paid to the exhaust port and vacuum port to avoid blockage, as well as to avoid blocking the head mouth die.

  • Pay attention to adjusting the screw combination of the twin screws to avoid high shear staying in the barrel for a long time.

More information about SINOYQX Melamine Cyanurate (MCA), please contact us via email: [email protected] , or voice to us at: +86-28-8411-1861.